180 Terms

1
New cards

High ADV sand in FURAN no-bake: effect?

Alkaline sand neutralizes the acid catalyst before curing → slow/incomplete cure, lower strength. Fix: lower-ADV sand or adjust catalyst; monitor with ADV test.

2
New cards

High ADV sand in PUNB: effect?

Alkaline sand SPEEDS the reaction → shorter work and strip time.

3
New cards

Low ADV (acidic) sand in PUNB: effect?

Slows the reaction → longer work/strip time.

4
New cards

High ADV sand in PUCB (cold box): effect?

Shortens bench life of the coated sand; tensile drops fastest with bench time (high ADV < lake sand < low ADV).

5
New cards

Three factors that limit PUCB bench life

Sand temperature, acid demand value (ADV), moisture content (blown air and dew point).

6
New cards

Moisture in FURAN no-bake: effect?

Dilutes the acid catalyst and slows cure rate; high humidity slows evaporation of the water given off.

7
New cards

Moisture in phenolic urethane: effect?

H2O reacts with Part II (isocyanate) to form a crystalline substance → less binder for bonding, lower strength, shorter bench life.

8
New cards

PUCB bench life vs sand moisture (chart)

≈2 h at 0–1% moisture, dropping to ≈0.3 h at 5% (30% tensile loss criterion).

9
New cards

Resin-sand moisture rule of thumb

≤0.2% H2O in winter, ≤0.1% in summer.

10
New cards

Sources of water in resin-bonded sand

Sand storage, binders, pattern surfaces, air humidity.

11
New cards

Effect of more moisture on resin sand tensile vs cure time

Lower final tensile strength and slower cure (curves for 0.0%, 0.3%, 1.0%).

12
New cards

10 °C rule

Each 10 °C (18 °F) rise doubles reaction speed; each 18 °F drop halves it.

13
New cards

Cold sand in PUNB: two effects

Reaction speed drops (halves per 18 °F) and resin viscosity rises → poorer coating, lower strength.

14
New cards

PU tensile vs sand temperature (1.25% PU chart)

Low at 50 °F, best around 80–100 °F, falls again when too hot (>~110 °F).

15
New cards

Furan: easier to control cure with ___ than with catalyst

Sand temperature.

16
New cards

Humidity fixes for phenolic urethane

Heat sand, warm or dry the pattern, put a drier on Part II.

17
New cards

Finer sand / more 140 mesh in a resin process: effect?

More surface area → more binder needed (~20×), lower permeability → more gas. In PU, more binder = more Part II N and C → pinholes, lustrous carbon.

18
New cards

1% on the 140 screen and finer: three effects

Reduces metal penetration, increases gas-related defects, requires more binder (more gases released).

19
New cards

Round-grain sand in furan: pros and caution

Coats better, uniform properties, higher compaction density. Caution: veining defects.

20
New cards

Angular vs rounded grains: binder

Angular = highest surface area and binder demand; rounded = lowest.

21
New cards

Why fine sand needs more binder

Fine grain surface area is ~20× greater than coarse grains.

22
New cards

Silica expansion: why high?

Quartz α→β inversion near 1063 °F (573 °C): sudden volume jump → veining, buckles, rat tails.

23
New cards

Rank sands by linear expansion (high → low)

Silica (0.018) > olivine (0.008) > chromite (0.005) > zircon (0.003).

24
New cards

PUCB sand additive for VEINING

Clay or iron oxide, 1–2%.

25
New cards

PUCB sand additive for EXPANSION and metal penetration

Gypsum-based, 5–10%.

26
New cards

PUNB defect-prevention additives (ferrous, esp. steel)

0.25–3% red iron oxide (hematite), 1–6% black iron oxide (magnetite), proprietary compounds (gypsum). Need more binder (surface area).

27
New cards

Benefits of iron oxide additions in PUNB

Minimize gas defects, control sand expansion defects, improve surface finish.

28
New cards

Resin-bonded sands: classified by process

No-bake, cold box, heat cured.

29
New cards

Resin-bonded sands: classified by curing mechanism

Acidic, basic (alkaline), other (neutral, dehydration, oxidation).

30
New cards

Causes of process variation in resin sands

Sand type, segregation, transport, temperature (patterns, reaction rate, resin blending), sticking, cycle times, moisture, humidity, sand additives, refractory coating (high moisture).

31
New cards

Thermoplastic vs thermoset

Thermoplastic softens on heating reversibly; thermoset cross-links into a rigid network that cannot re-melt.

32
New cards

Furan binder reaction

Furan resin (Part I) + acid catalyst (Part II) → furan binder + H2O.

33
New cards

Furan resin basic component

Furfuryl alcohol.

34
New cards

Furan resin graded by

Nitrogen (0–11%) and water (0–30%); lower content = higher grade.

35
New cards

Effects of more furfuryl alcohol

Better environmental, casting and process performance; higher cost.

36
New cards

Three functions of furan acid catalyst

1) Neutralize alkaline contaminants 2) Initiate cross-linking 3) Sustain condensation cure.

37
New cards

Furan condensation cure characteristics

Slow cure rate; cures from outside inward. Concentrated acid → optimized rate and deep-set properties.

38
New cards

Furan acid catalysts, least → most reactive

75% phosphoric, 85% phosphoric, toluene sulfonic, xylene sulfonic, benzene sulfonic.

39
New cards

Furan mixing order

Catalyst FIRST, mixed thoroughly; resin added slowly next. NEVER mix catalyst and resin together — exothermic, explosion.

40
New cards

Furan resin and catalyst levels

Resin 0.9–2.0% BOS; catalyst 30–50% BOR.

41
New cards

Furan work time vs strip time

Work time = 50–60% of strip time; strip 1–30 min; 70–90% of properties developed in 3 hours.

42
New cards

Furan: when to apply refractory coating

AFTER deep-set properties develop; earlier → incomplete cure (water-based, non-permeable).

43
New cards

Which sands neutralize furan catalyst

High-ADV sands: some silica, olivine.

44
New cards

Furan casting properties

Excellent dimensional accuracy; resists veining, erosion, penetration; high tensile; excellent hot properties; decomposes completely → good shakeout.

45
New cards

Furan advantages

Lower smoke/odor, wider binder ranges, color change indicates cure, excellent flowability, agricultural by-products.

46
New cards

Furan disadvantages

Nitrogen and sulfur residues, raw material shortages, acidic grain surface, mechanical reclamation.

47
New cards

Ester-cured alkaline phenolic: components

Phenolic RESOLE resin + liquid ester co-reactant (H in alcohol radical replaced by Na or K).

48
New cards

Ester-cured phenolic levels

Resin 1.0–1.5% BOS; co-reactant 20–25% BOR.

49
New cards

Ester-cured phenolic advantages

Lower smoke/odor, easy stripping, good finish, low veining, minimal erosion, excellent hot strength, water-based resin.

50
New cards

Ester-cured phenolic disadvantages

High viscosity, poor flowability and compaction, low strength, limited storage life, poor reclamation, shakeout problems.

51
New cards

Shell (Croning) resin and curing agent

Phenolic NOVOLAK + hexamethylenetetramine (hexa).

52
New cards

Shell hot-coat temperatures

Resin in at 320 °F → quench water/hexa at 275 °F → 'break' at 200 °F → aerate and discharge at 160 °F.

53
New cards

Shell resin curing phases

1) Thermoplastic: heat and melt 2) Transitional: flow and cure (gel) 3) Thermoset: fused solid, postcure. Overbake → decompose.

54
New cards

Shell process steps

Dump/blow into heated box → build 1/8–1/2 in. shell → rotate to drain unreacted sand → dwell to cure through → strip/eject.

55
New cards

Shell die temperature range

450–525 °F, kept uniform (position gas burners strategically).

56
New cards

Shell peelback cause

Zone temperature too LOW (cold area of the die).

57
New cards

Shell additive: iron oxide

Reduces thermal cracking, provides chill, minimizes gas defects.

58
New cards

Shell additive: potassium fluoroborate

Added for magnesium castings.

59
New cards

Shell additive: kaolinite clay

Improves hot strength, provides chill, eliminates orange peel on steel castings.

60
New cards

Shell additive: plasticizers

Reduce thermal cracking.

61
New cards

Shell process advantages

Waste minimization, easily reclaimed, superior finish, excellent tolerances, low gas emission.

62
New cards

PUNB Part I

Phenolic polyol dissolved in organic solvents.

63
New cards

PUNB Part II

Polymeric MDI-type isocyanate dissolved in solvent. Contains ALL the nitrogen.

64
New cards

PUNB Part III

Amine-type catalyst; initiates reaction and is NOT consumed.

65
New cards

PUNB binder and catalyst levels

Binder 0.8–1.75%; catalyst 2–9%.

66
New cards

PU ideal vs recommended Part I:II ratio

Ideal properties at 50:50; recommended 55:45 to reduce N pinholes and lustrous carbon, but ultimate strength drops.

67
New cards

Why favor Part I in phenolic urethane?

Part II has all the nitrogen and more carbon → nitrogen pinholes in iron, lustrous carbon defects.

68
New cards

PUNB: how to add catalyst in batch production

Add catalyst after mixing with Parts I and II, or blend catalyst into Part II. Uneven catalyst → hot spots and soft areas.

69
New cards

Source of VOCs in PUNB

Catalyst and solvents.

70
New cards

Pattern practice for PU no-bake

Do not paint pattern; use organic-based release agents; spray and wipe down; clean tooling periodically.

71
New cards

Strip/work time chart: effect of catalyst speed

High-speed catalyst moves work and strip time earlier; slow catalyst later.

72
New cards

PUCB processing steps in order

Coat sand with Parts I & II → blow → gas (tertiary amine) → purge (dry air) → amine to scrubber → remove core.

73
New cards

PUCB blow pressure

35–65 psi.

74
New cards

PUCB gas vs purge pressure

Amine gas LOW 5–20 psi; dry-air purge HIGH 20–60 psi.

75
New cards

Effect of a longer PUCB blow cycle

Does NOT increase density; causes resin wipe-off, parting-line blowout, sticking to core box.

76
New cards

Purpose of PUCB purge cycle

Distribute and complete cure, remove amine gas.

77
New cards

What the PUCB scrubber does

Converts amine gas into an inert acid salt.

78
New cards

Amine concentration in carrier gas

6–12%.

79
New cards

Too little vs too much amine

Too little → under-cured cores. Too much → higher cost and odor.

80
New cards

DMEA vs TEA vapor pressure

DMEA 435 mm vs TEA 54 mm (liquid at 20 °C).

81
New cards

TEA vs DMEA carrier gas

TEA needs 7.8× as much carrier gas to deliver the same amount of amine.

82
New cards

PUCB: water-based coating practice

Apply as soon as possible (interrupts curing); dry immediately at 250 °F in a convection oven.

83
New cards

Lustrous carbon fixes (cold box)

55:45 ratio, lower resin content, higher pour temp, shorter pour time, venting, 1–3% iron oxide.

84
New cards

PUCB resin additives do what?

Enhance casting properties, improve release, moisture resistance, extend bench life, lower VOCs; bio-diesel (dimethyl ester) improves shakeout.

85
New cards

Factors for optimal amine use

Gas concentration, gas and purge volume, line size, catalyst/purge temperature, tooling venting and sealing, exhaust area, direct exhaust to scrubber.

86
New cards

Six molding process selection factors

Casting complexity and size, production run, process costs, dimensional accuracy/tolerances, mechanical properties, alloy type.

87
New cards

Aggregate characteristics (list)

Thermal/dimensional stability, suitable size and shape, chemically stable, non-wetting, economical, doesn't degrade in volatile gases, uniform and pure, appropriate chemistry, binder compatible.

88
New cards

Fine vs coarse grains: permeability

Fine restricts gas paths (low permeability); coarse gives high permeability.

89
New cards

Fine vs coarse grains: surface finish

Fine = better finish; coarse = poorer finish and more metal penetration.

90
New cards

Fine grains and heat

Soften sooner: good for expansion, bad for stability.

91
New cards

Ideal sand distribution goals

Coarse + fine + medium (bulk) grains → optimize compaction, adequate permeability, optimal strength, minimum binder, prevent agglomeration.

92
New cards

AFS distribution: which screens count?

Screens holding 10% or more.

93
New cards

Grain shapes (4)

Rounded, sub-angular, angular, compounded (little grains stuck together).

94
New cards

Segregation: coarse vs fine particles

Coarse: more mass and momentum. Fine: less mass and momentum.

95
New cards

Segregation: rounded vs angular

Rounded tend to roll (less energy); angular tend to slide (more energy).

96
New cards

Where segregation causes problems

Sand transfer, binder coating, core blowing, green sand mulling.

97
New cards

ADV test determines

Acidic or basic components in sand; matters for binder levels and thermal reclamation.

98
New cards

Durability of sand means

Survives thermal shock (pouring, cycling), crushing/splitting under load, surface wear in transport.

99
New cards

Higher sand density effects

Stronger cores/molds, larger mass, lower permeability, possible expansion defects. Lower density → more metal penetration.

100
New cards

Sand temperature effects

Green sand: rapid moisture loss, degraded properties. Some resins: interferes with bonding.