Chapter One Section(10) Arc Welding Flaws, Cracking, and Discontinuities

Arc Welding Flaws and Porosity

  • Weld soundness depends heavily on welder technique, including directing the arc to the proper location and correctly adjusting work and travel angles.

  • Porosity is caused by trapped gases in the weld metal, appearing as surface porosity (Figure 1.34) or subsurface porosity (Figure 1.35).

  • Common causes of porosity include inadequate shielding gas flow, atmospheric drafts, excessive work distance, clogged nozzles, leaks in the gas line, contaminated wire, worn O-rings, and improper arc length.

  • Methods to avoid porosity include removing rust from the joint area, ensuring joint cleanliness, and keeping flux clean and dry.

Weld Cracking Mechanisms

  • Solidification Cracking (Hot Cracking): Occurs at elevated temperatures during welding along the length or center line of a weld (Figure 1.36); associated with PDAW, SMW, and SAW, especially when deposited over large panels.

  • Solidification cracking is mitigated by improving travel speed and increasing root opening to reduce dilution from higher-carbon base materials.

  • Cold Cracking: Occurs at low temperatures hours, days, or months after weld completion, primarily caused by absorbed hydrogen in the weld metal.

Hydrogen Control and Inclusions

  • Hydrogen Mitigation: Countered by post-weld heating to allow hydrogen gas to escape from solidified weld metal, proper joint preparation, dry electrode storage, and using spray transfer mode instead of short-circuiting or globular metal transfer.

  • Tungsten Inclusions: Discontinuities introduced directly into the weld metal from the tungsten electrode.

  • Slag Inclusions: Occur in flux-based processes (SMPW, SMAW, FCAW, and SAW); prevented by thorough interpass slag removal, proper weld bead contouring, and avoiding highly convex shapes by increasing voltage.

Incomplete Penetration, Incomplete Fusion, and Undercut

  • Incomplete Fusion and Incomplete Joint Penetration: Common along groove faces during short-circuit GMAW transfer mode (Figure 1.37).

  • Causes include improper electrode alignment with the joint, incorrect polarity, excessive electrical stickout, or long work distance.

  • Prevention methods include using adequate welding current for the joint design, back gouging down to sound metal, reducing contact-to-work distance, and using shielding gas mixtures with higher CO2CO_2 content for a broader penetration profile.

  • Undercut: Caused by excessive voltage, incorrect electrode position, or excessively slow travel speed; controlled by managing voltage, current, electrode angles, travel speed, gun control, and dwell time.