Comprehensive Study Guide for Bulk Metal Forming and Machining

Fundamental Classification of Metal Working Processes

  • Criteria for Classification:
    • Based on Final Product: Bulk forming and Sheet forming.
    • Based on Surface Area to Thickness Ratio: This distinguishes between bulk forming (low ratio) and sheet metal forming (high ratio).
    • Based on Loading Conditions:
      • Direct compression type processes (e.g., Forging, Rolling).
      • Indirect-compression processes (e.g., Extrusion, Drawing).
      • Tension type processes.
      • Bending processes.
      • Shearing processes.
    • Based on Working Temperature:
      • Cold working (TH<0.3T_H < 0.3).
      • Warm working (0.3≤TH≤0.50.3 \le T_H \le 0.5).
      • Hot working (TH>0.5T_H > 0.5).
      • Homologous Temperature (THT_H): The ratio of a material's absolute operating temperature (TT) to its absolute melting temperature (TmT_m), both in Kelvin (TH=TTmT_H = \frac{T}{T_m}).
    • Based on Process Order: Primary mechanical working (breaking down ingots) and Secondary mechanical working (shaping near-finished parts).

Common Starting Materials in Metal Forming

  • Bloom: A material with a square or rectangular cross-section. Its thickness is greater than 150 mm150\,mm, and its width is no greater than twice the thickness.
  • Billet: A material with a square or circular cross-section. It is smaller than a bloom, typically with dimensions of 40 mm40\,mm on a side or more.
  • Slab: A rectangular shape where the width is greater than twice the thickness. Slabs are rolled into plates, sheets, and strips. Standard dimensions include width of 250 mm250\,mm or more and thickness of 40 mm40\,mm or more.

Introduction to Forging

  • Definition: Forging is the process of shaping materials through hammering or pressing. It is one of the oldest metalworking processes, originating from primitive blacksmithing.
  • Temperature Ranges: Usually carried out at high temperatures (hot forging), though it can rarely be performed at room temperature (cold forging).
  • Mechanical Benefits:
    • Refines grain structure and improves physical properties.
    • Creates controlled development of grain flow lines that follow the outline of the component.
    • Continuous grain flow increases overall toughness and reduces susceptibility to fatigue and corrosion failures.
  • Deformation Modes:
    • Drawn out: Increases length, decreases cross-section.
    • Upset: Decreases length, increases cross-section.
    • Squeezed: Conducted in closed impression dies to compel multi-directional flow into a desired shape.
  • Forgeability: The capability of a metal to undergo deformation without cracking.
    • Ability to cold forge depends on ductility and malleability.
    • Ability to hot forge depends on the "range of plasticity" at high temperatures.

Metals and Forging Temperatures

  • Process Suitability:
    • Low and medium carbon steels: Easily forged.
    • High carbon and alloy steels: Difficult to forge.
    • Cast Iron: Not forgeable.
  • Average Forging Temperatures:
    • Steels: 1100 ∘C to 1250 ∘C1100\,^\circ C \text{ to } 1250\,^\circ C.
    • Copper Alloys: 750 ∘C to 950 ∘C750\,^\circ C \text{ to } 950\,^\circ C.
    • Aluminum Alloys: 350 ∘C to 500 ∘C350\,^\circ C \text{ to } 500\,^\circ C.
    • Magnesium Alloys: 250 ∘C to 400 ∘C250\,^\circ C \text{ to } 400\,^\circ C.

Forging Operations and Specialized Techniques

  • Upsetting: A solid workpiece is placed between two flat dies and reduced in height while increasing in lateral size. Friction at the die-work interface opposes spreading at the surfaces, leading to Barreling (a barrel-shaped expansion in the center). Lubrication reduces this effect.
  • Edging: Shapes the ends of bars and gathers metal using a concave open-die. Flow is confined horizontally but free laterally to fill the die.
  • Cogging (Drawing Out): An open-die operation where the thickness of a bar is reduced by successive hammer blows at specific intervals.
  • Fullering: Reduces the cross-sectional area of a portion of the stock. Metal flows outward away from the center. Fuller dies are usually convex. Example: Forging of internal-combustion engine connecting rods.
  • Coining: A closed-die forging process used for coins and jewelry. High pressures (5-6 times material strength) are required. Lubricants are avoided because they are incompressible and prevent fine detail reproduction.
  • Rotary Swaging: Used to reduce the diameter of round bars or tubes. The workpiece is stationary while dies rotate in a housing, striking the metal at 10−2010-20 strokes per second. Internal mandrels control tube thickness or internal diameter.
  • Orbital Forging (Rotary Forging): Uses two dies to deform only a small portion of the workpiece at once. The upper die axis is tilted; as it rotates, it applies a sweeping line of pressure rather than striking the whole surface. Ideal for large-diameter flanges (e.g., bevel gears, wheel disks).
  • Flashless Forging (Precision Forging): The metal is totally confined in a cavity. It eliminates scrap from flash formation. Requires accurate workpiece positioning, good die design, and precise lubrication.
  • Piercing: Metal flows around a moving die as it pierces the surface.
  • Punching: A cutting operation producing a hole using a punching die.

Forging Equipment and Classification

  • Hand Forging: Shaping heated metal by repeated strokes of a handheld hammer on an anvil.
  • Drop Forging (Hammer): A mechanized form of blacksmithing. A massive weight (ram) is raised and dropped. Hammers use compressed air or steam to lift the ram, which falls by gravity. Final shapes are achieved in multiple steps via repeated blows.
    • Power Hammer: Provides greater capacity as the ram is accelerated on the downstroke by air/steam pressure in addition to gravity.
    • Energy Equation (Power Hammer): W=12mv2+pAH=(mg+pA)HW = \frac{1}{2}mv^2 + pAH = (mg + pA)H.
  • Press Forging: Uses a slow squeezing action rather than impact. It is more accurate and quieter than drop forging, transferring force uniformly and gradually. Deeper penetration is achieved.
    • Hydraulic Presses: Load-restricted; pressure moves a piston. Full load is available at any point in the stroke. Well-suited for extrusion-type forging.
    • Mechanical Presses: Stroke-restricted; reciprocating linear motion. Rated based on force at the end of the stroke.
    • Energy Equation (Mechanical Press): W=12I(ω02−ωf2)W = \frac{1}{2}I(\omega_0^2 - ω_f^2).

Open-Die vs. Closed-Die Forging

  • Open-Die Forging:
    • Performed between flat dies or simple shapes.
    • Used for large parts in small quantities.
    • Low cost for dies, but quality depends on operator skill.
    • Often used to make preforms for closed-die forging.
  • Closed-Die (Impression-Die) Forging:
    • Metal is deformed under high pressure between die halves with specific impressions.
    • The billet flows to fill the cavity completely.
    • Flash: Excess metal squeezed into the narrow gap at the parting line. It acts as a safety valve and builds high internal pressure to ensure the metal fills all die recesses.
    • Flash Land: Restricts flow to help build pressure.
    • Gutter: Collects excess flash.

Force-Stroke Analysis in Closed-Die Forging

  • Phase 1: Initial Contact: Low, gradual force increase as the die touches the billet.
  • Phase 2: Flash Initiation: Force rises faster as the cavity fills and excess metal extrudes into the flash land.
  • Phase 3: Complete Filling (Peak Load): Force shoots up vertically. Friction and rapid cooling in the thin flash gap restrict sideways flow, forcing metal into tight die corners.

Forging Die Design and Materials

  • Required Material Properties: High strength and toughness at high temperatures, uniform hardenability, resistance to mechanical/thermal shock, and wear resistance.
  • Common Materials: Tool steels with Chromium (CrCr), Nickel (NiNi), Molybdenum (MoMo), and Vanadium (VV). Alloyed steels for high-temperature presses; medium-alloyed for hammers.
  • Design Rules:
    • Symmetrical dies (spherical or block-like) facilitate better flow.
    • Avoid sharp changes in section.
    • Draft Allowance: Required to remove parts. Typically 3−5∘3-5^\circ for outside surfaces and 7−10∘7-10^\circ for inside surfaces.
    • Fillets: Generous radii are necessary.
    • Counterlock: Prevents dies from sliding apart due to side thrust.

Forging Defects and Residual Stresses

  • Unfilled Section: Die sections not completely filled due to improper design or technique.
  • Die Shift: Misalignment of die halves causes improper shape.
  • Scale Pits: Irregular indentations caused by oxides/scales embedded in the surface during forging.
  • Cold Shut: Small cracks at corners caused by small radii preventing proper metal flow.
  • Flakes: Internal ruptures caused by improper cooling of large forgings. Rapid cooling causes exterior contraction and internal fractures (often associated with high hydrogen content).
  • Residual Stresses: Appreciable stresses and warping can occur during quenching. Large forgings must be cooled slowly (e.g., buried in ashes for weeks) to prevent flaking.

Analysis of Open-Die Forging Mechanics

  • Ideal Deformation (No friction):
    • True Strain: ϵ=ln⁡(h0h)\epsilon = \ln\left(\frac{h_0}{h}\right).
    • Forging Force: Ffg=σfAF_{fg} = \sigma_f A.
    • Flow Stress: σf=Kϵn\sigma_f = K\epsilon^n.
    • Volume Constancy: A0h0=AhA_0 h_0 = Ah.
  • Actual Deformation (With Friction):
    • Friction causes barreling, especially in hot working with cold dies.
    • Shape Factor (KfK_f): Kf=1+0.4μDhK_f = 1 + \frac{0.4\mu D}{h}.
    • Actual Forging Force: Ffg=KfσfAF_{fg} = K_f \sigma_f A.

Introduction to Rolling

  • Definition: Plastically deforming metals by passing them between rolls.
  • Loading: High compressive stresses from roll squeezing and surface shear stresses from friction.
  • Hot Rolling: Performed above recrystallization temperature (T>TRecryT > T_{Recry}). Offers high deformation, minimum residual stresses, and isotropic properties. Disadvantages include an oxide layer and lower precision.
  • Cold Rolling: Performed below recrystallization temperature (T<TRecryT < T_{Recry}). Offers high precision, superior surface finish, and increased strength/hardness via work hardening. Only ductile metals are suitable.

Rolling Mill Types

  • Two-High Mill: Simplest form; rolls rotate in opposite directions. Vertical gap is adjustable.
  • Two-High Reversing Mill: Rolls can reverse direction so work can pass back and forth for successive reductions.
  • Three-High Mill: Three vertical rolls; direction of each remains unchanged. Work passes one way through the bottom pair and returns through the top pair.
  • Four-High Mill: Two small-diameter work rolls backed by two large-diameter rolls. Small work rolls reduce roll force and allow rolling of thin sheets to close tolerances.
  • Cluster Mill (Sendzimir Mill): Each work roll is supported by multiple backing rolls for extreme rigidity.
  • Tandem Mill: A series of rolling stands in a line. Speed is synchronized so each stand takes the strip at the delivery speed of the previous one.
  • Universal Rolling Mill: Consists of two vertical rolls (idle) and two horizontal rolls. Used for producing H-section beams and blooms from ingots.
  • Planetary Mill: A pair of heavy backing rolls surrounded by many small planetary rolls. Reduces a slab to a strip in a single pass.

Analysis of Rolling Mechanics

  • Draft (Δt\Delta t): The thickness reduction per pass, Δt=ti−tf\Delta t = t_i - t_f.
  • Angle of Bite (Contact Angle, α\alpha): The angle defining the arc of contact.
  • Condition for Biting: Rolling occurs only if μ≥tan⁡(α)\mu \ge \tan(\alpha).
  • Maximum Draft: Δtmax=μ2R\Delta t_{max} = \mu^2 R.
  • Contact Length (LL): L≈RΔtL \approx \sqrt{R \Delta t}.
  • Velocity Relationships:
    • Entry (ViV_i): Vi<VrV_i < V_r (Backward slip).
    • Neutral Point: Vstrip=VrV_{strip} = V_r (No-slip point).
    • Exit (VfV_f): Vf>VrV_f > V_r (Forward slip).
  • Rolling Force Calculation:
    • For ideal plastic material: F=σysLbF = \sigma_{ys} L b.
    • For strain-hardening material: F=σavgLbF = \sigma_{avg} L b, where σavg=Kϵn1+n\sigma_{avg} = \frac{K\epsilon^n}{1+n}.
  • Torque and Power:
    • Torque (TT): T=F×αLT = F \times \alpha L, where arm length is approximately 0.5L0.5L.
    • Power (PP): P=2×2πNT60P = 2 \times \frac{2\pi NT}{60} Watts (for two driven rolls).

Rolling Phenomena and Defects

  • Friction Hill: Pressure rises to a maximum at the neutral point and then falls off. The area under the hill is proportional to the rolling load.
  • Tension Effects:
    • Back Tension: Tensile force on the entry side.
    • Front Tension: Tensile force on the exit side.
    • Benefit: Both reduce the compressive roll pressure required for plastic deformation, effectively lowering the rolling load. Back tension is generally more effective than front tension.
  • Defects:
    • Wavy Edges: Edges elongate more than the center due to roll bending.
    • Edge Cracks: Caused by excessive reduction or incorrect temperatures.
    • Zipper Cracks: Cracks at the centerline due to poor ductility.
    • Alligatoring: Workpiece splits into two layers. Caused by non-uniform deformation or internal defects.

Extrusion Processes

  • Definition: An indirect compressive process where a metal block is forced through a die opening to produce a uniform cross-section.
  • Types:
    • Direct Extrusion (Forward): Ram and billet move in the same direction. High friction between billet and container.
    • Indirect Extrusion (Backward): A hollow ram carries the die. Billet does not move relative to the container, resulting in lower friction and less force. Practical limit: ram strength.
    • Hydrostatic Extrusion: Container filled with fluid transmits pressure to the billet. Eliminates contact friction. Suitable for brittle materials.
    • Impact Extrusion: High-speed striking of a slug, often at room temperature, for short hollow shapes (e.g., collapsible tubes).
  • Extrusion Ratio (rxr_x): rx=A0Afr_x = \frac{A_0}{A_f}.
  • Extrusion Strain (ϵx\epsilon_x): Estimated using Johnson’s formula: ϵx=a+bln⁡(rx)\epsilon_x = a + b \ln(r_x), where a≈0.8a \approx 0.8 and b≈1.2 to 1.5b \approx 1.2 \text{ to } 1.5.
  • Defects:
    • Chevron Cracking (Center-burst): Internal cracks due to hydrostatic tensile stress at the centerline.
    • Piping (Tailpipe/Fishtailing): Void created at the end of the billet due to surface impurities and oxides flowing into the center.
    • Surface Cracking: Intergranular cracks caused by excessive speed or friction inducing high temperatures.

Drawing Processes

  • Definition: Pulling metal through a die using a tensile force applied to the exit side. Indirect compression is caused by the reaction with the die.
  • Types:
    • Rod/Bar Drawing: Single-stage operation for large diameters.
    • Wire Drawing: Continuous drawing through a series of 44 to 1212 dies from large coils. "Wire" usually refers to diameters under 5 mm5\,mm.
    • Tube Sinking: Drawing a tube without a mandrel; no control over wall thickness.
    • Fixed Mandrel Drawing: Controls internal diameter/thickness but limited by the support bar length.
    • Floating Mandrel Drawing: A plug floats in the die throat. Allows for longer tubes and less load than fixed mandrels.
    • Moving Mandrel Drawing: A long rod moves with the tube, minimizing friction.
  • Drawing Die Geometry:
    • Bell-shaped mouth: Lubricant entry.
    • Approach angle: Actual reduction zone (6∘ to 20∘6^\circ \text{ to } 20^\circ).
    • Bearing region: Sizes the final product.
    • Back relief: Allows slight expansion (25∘ to 30∘25^\circ \text{ to } 30^\circ).
  • Drawing Stress (σd\sigma_d): σd=σavg(1+μα)ϕln⁡(A0Af)\sigma_d = \sigma_{avg} (1 + \frac{\mu}{\alpha}) \phi \ln\left(\frac{A_0}{A_f}\right).
    • ϕ\phi factor accounts for inhomogeneous deformation: ϕ=0.88+0.12(DLc)\phi = 0.88 + 0.12 \left(\frac{D}{L_c}\right), where DD is average diameter and LcL_c is contact length.

Questions & Discussion

  • GATE 2011 Question: The maximum possible draft in cold rolling of sheet increases with the: (a) increase in coefficient of friction (b) decrease in coefficient of friction (c) decrease in roll radius (d) increase in roll velocity. Answer: (a).
  • Numerical Example (Draft): Determine max reduction for cold-rolling a 300 mm300\,mm thick slab (μ=0.08\mu=0.08, Roll Diameter=600 mm600\,mm). Answer: Δtmax=(0.08)2×300=1.92 mm\Delta t_{max} = (0.08)^2 \times 300 = 1.92\,mm. For hot rolling (μ=0.5\mu=0.5): Δtmax=(0.5)2×300=75 mm\Delta t_{max} = (0.5)^2 \times 300 = 75\,mm.
  • GATE 2015 Question: If a 25 mm25\,mm thick plate cannot be reduced to less than 20 mm20\,mm in one pass with roll diameter 500 mm500\,mm, find μ\mu. Answer: μ=25−20250≈0.1414\mu = \sqrt{\frac{25-20}{250}} \approx 0.1414.
  • Numerical Example (Forging Force): Cylindrical piece (h0=75 mmh_0=75\,mm, D0=50 mmD_0=50\,mm) reduced to h=36 mmh=36\,mm. K=350 MPaK=350\,MPa, n=0.17n=0.17, μ=0.1\mu=0.1. At final height (h=36 mmh=36\,mm): ϵ=ln⁡(75/36)=0.734\epsilon = \ln(75/36) = 0.734. Yf=350(0.734)0.17=332.1 MPaY_f = 350(0.734)^{0.17} = 332.1\,MPa. Area A=4094.2 mm2A = 4094.2\,mm^2. Kf=1+0.4(0.1)(72.2)/36=1.08K_f = 1 + 0.4(0.1)(72.2)/36 = 1.08. Force F=1.08×332.1×4094.2=1468.5 kNF = 1.08 \times 332.1 \times 4094.2 = 1468.5\,kN.